API 6A Bolting Torque for Flanges (USC Units)

This table gives the recommended make-up torque for API 6A flange bolting from API 6A (21st edition) Annex H, Table H.2 (USC units), for ASTM A453 Grade 660 Class D studs with Sy = 105 ksi tightened to a bolt stress of 52.5 ksi, half the yield strength. Torque applied to a nut is only one way to approximate stud tension: lubrication, thread and nut-face condition change the result (H.3). The same values are on the SI units page.

Stud Diameter D in. Threads per in. N 1/in. Studs with Sy = 105 ksi
Bolt Stress Equal to 52.5 ksi
Tension F lbf Torque f = 0.07 ft-lbf Torque f = 0.13 ft-lbf
0.500 13 7,450 35 59
0.625 11 11,865 68 115
0.750 10 17,559 118 200
0.875 9 24,241 188 31 9
1.000 8 31 ,802 279 474
1.125 8 41,499 401 686
1.250 8 52,484 553 953
1.375 8 64,759 739 1281
1.500 8 78,322 962 1677
1.625 8 93,1 73 1226 21 46
1.750 8 109,313 1534 2696
1.875 8 126,741 1890 3332
2.000 8 145,458 2297 4061
2.250 8 186,758 3276 5822
2.500 8 233,21 2 4500 8030
2.625 8 - - -
2.750 8 - - -
3.000 8 - - -
3.250 8 - - -
3.750 8 - - -
3.875 8 - - -
4.000 8 - - -

What does ASTM A453 Grade 660 Class D require?

ASTM A453 Grade 660 Class D is solution treated at 1650 ± 25 °F [900 ± 14 °C] for 2 h min or 1800 ± 25 °F [980 ± 14 °C] for 1 h min and liquid quenched, then aged at 1325 ± 25 °F [720 ± 14 °C] for 16 h and air cooled, with a second age at 1200 ± 25 °F [650 ± 14 °C] for 16 h if needed to reach the properties (A453/A453M-17 Table 4). Table 5 requires up to 2½ in. [63.5 mm]: 130 ksi [895 MPa] tensile and 105 ksi [725 MPa] yield; over 2½ in. [63.5 mm]: 120 ksi [825 MPa] tensile and 95 ksi [655 MPa] yield; 15 % elongation, 18 % reduction of area and 248 to 321 HB (24 to 35 HRC) in both size ranges.

Class D does not require a stress-rupture test and is stamped NR in addition to the other required markings (8.2.1, 9.1). Each bolting component carries the grade symbol and class (660 D) and the thread type: M1 or M2 for machined threads, R1 or R2 for rolled threads, formed after (1) or before (2) the precipitation heat treatment (6.1.1, 9.1). The 35 HRC maximum matches the ISO 15156-3 (NACE MR0175) limit for UNS S66286. API 20F covers Grade 660 Class D for BSL-2 and BSL-3 bolting, and API 6A (21st edition) 8.2.3.6 cautions against Grade 660D on pressure-containing connectors in salt-air offshore or coastal service, or where equipment is washed with raw seawater. See the ASTM A453 660D (Class D) specification, ASTM A453 Grade 660 chemical composition and mechanical properties.

Same table in SI units: API 6A Bolting Torque for Flanges (SI Units). Stud forms: ASTM A453 Grade 660 Class D API 6A Full Thread Stud Bolt, ASTM A453 Grade 660 Class D API 6A Tap End Stud Bolt.

Source: ASTM A453/A453M-17; API 6A 21st edition; API 20F; ISO 15156-3. Last reviewed .

Specifications
  • ASTM A453
  • ASTM A638
  • EN 10269
  • EN 10083-3
  • ISO 3506-5
  • DIN 267
Surface Treatments
  • Xylan 1070 / 1014 / 1400 / 1424
  • Xylar 2 / 101
  • SermaGard 1105 / 1280
  • Dacromet 320 / 500
  • TakeCoat 1000 Ceramic
  • Magnigard
  • MolyKote
Certifications
  • ISO 9001 - 2015 Certified
  • PED 2014/68/EC
  • NACE MR0175/ISO 15156-2
  • NORSOK M-650
  • DFAR
  • MERKBLATT AD 2000 W2/W7/W10